1) Temperature during heat absorption: PE80 national standard 210 degrees / plus or minus 10 degrees. British standard 233 degrees / plus or minus 3 degrees; PE100 national standard 225 degrees / plus or minus 10 degrees.
2) Welding time: SDR11 national standard pipe diameter ÷ 11 × 10 = welding time, SDR 17.6 national standard pipe diameter ÷ 17.6 × 10 = welding time,
Cooling time: 90-315SDR11: 11, 14, 19, 23, 28, 35 minutes. British standard has another calculation formula,
There is a big difference between the calculated time and the national standard, especially the cooling time.
3) Pressure: The national standard is drag pressure heat absorption, the British standard is pressure heat absorption, drag pressure + welding pressure = butt pressure;
Drag pressure: it is the pressure at which the pipe can be dragged when the machine is running.
Welding pressure: the pressure given by the national standard ÷ the cross-sectional area of the welding machine cylinder = the welding pressure. For example: the pressure given by the 90mm national standard is 3.15MPa, and the cross-sectional area of the cylinder is 10 square centimeters, that is 3.15÷10=0.315MPa,
The pressure given by the national standard: It seems to remember that 90 is 3.15, 110 is 4.71, 160 is 9.96, and 250 is 24.33, (unit/MPa)
In addition, there are requirements for the height and width of the crimping (protrusion). As long as these requirements are met, the weld will be very good. However, since the automatic hot melt welder is used, it should be in the welder. Do you have these parameters? No manual calculation is required. Unless you are blinded by someone, if you are not fully automatic, it is also said to be fully automatic.